A gradient-index glass rod of about 13 mm in diameter and 20 mm in length with the
refractive index difference of about 0.05 between center and perimeter has been
prepared by the sol-gel process from a precursor solution consisted of
tetramethoxysilane, tetraethoxysilane, boron ethoxide and aqueous solution of lead
acetate. A bubble free wet gel of about 35 mm in diameter and 50 mm in length was
obtained by adding acetic acid to the precursor solution as a buffering agent. The
liquid in the micropores of the wet gel was totally replaced with acetone. Then the
compositional gradient of lead was formed in radial direction of the gel by soaking
in an ethanolic solution of potassium acetate. A transparent r-GRIN rod of about
13 mm in diameter was obtained by sintering the gel at 550°C.
Masayuki Yamane,Atsuo Yasumori,Mitsunobu Iwasaki, andKazutaka Hayashi
"Graded index materials by the sol-gel process", Proc. SPIE 1328, Sol-Gel Optics, (1 November 1990); https://doi.org/10.1117/12.22553
ACCESS THE FULL ARTICLE
INSTITUTIONAL Select your institution to access the SPIE Digital Library.
PERSONAL Sign in with your SPIE account to access your personal subscriptions or to use specific features such as save to my library, sign up for alerts, save searches, etc.
The alert did not successfully save. Please try again later.
Masayuki Yamane, Atsuo Yasumori, Mitsunobu Iwasaki, Kazutaka Hayashi, "Graded index materials by the sol-gel process," Proc. SPIE 1328, Sol-Gel Optics, (1 November 1990); https://doi.org/10.1117/12.22553